Short answer: TPU prints reliably on every current Bambu Lab printer once you get three things right — dry the spool properly, match the feeding path to the filament's Shore hardness, and slow the print down. Run the nozzle at 220–240°C with a low bed temperature of around 30–45°C, and use 0.8–1.2 mm of retraction, which suits the direct-drive extruders fitted to the whole Bambu Lab range. Get those basics in place and flexible parts come out clean on anything from an A1 Mini to an H2 series machine.
Why TPU behaves differently to rigid filament
TPU (thermoplastic polyurethane) is a flexible filament, and flexibility is exactly what makes it awkward to print. A rigid filament like PLA acts as its own pushrod: the extruder gears grip it and the whole strand transmits that force straight into the hotend. TPU behaves more like a wet noodle — push it too hard or too fast and it buckles, wraps around the drive gears, or compresses and oozes unpredictably. Every TPU problem you will meet (jams, blobs, stringing, inconsistent extrusion) traces back to either that buckling or to moisture, which is why feeding path and drying matter more here than for any rigid material. If you are still deciding whether TPU is even the right material for the job, start with our filament selection guide for Australia.
Step 1: Pick the right Shore hardness first
"TPU" is not one material — it is a hardness ladder, and the grade you pick determines how you must feed it. From firmest to softest in the Bambu Lab range: TPU for AMS at Shore 68D (semi-rigid, roughly the feel of a hard shell suitcase), then TPU 95A HF (about the firmness of a tyre tread), TPU 90A, and TPU 85A (soft shoe-sole territory). The softer the grade, the more rubber-like the part — and the harder it is to push through a long filament path. We cover the A/D scales, what each grade actually feels like, and which to buy for which job in our dedicated TPU Shore hardness guide.
One correction worth making early, because it saves people buying the wrong spool: hardness is not the same thing as rebound. A soft TPU deforms easily but does not necessarily spring back with energy. If what you actually want is bounce — toy wheels, balls, impact returns — a dedicated high-rebound material like BIQU PLA-HR is the better tool, and it feeds like a normal rigid filament.
Step 2: Dry it — not optional in Australia
TPU is strongly hygroscopic, and most Australians live on the coast where 60–80% relative humidity is normal. A TPU spool left in open air for even a few days will hiss and pop in the nozzle, string badly, and produce rough, bubbly surfaces. Dry TPU at around 70°C for 8 hours or more before a big job, and store it sealed with desiccant between prints — our filament storage guide for Australian conditions covers dry boxes and drying hardware in detail. If you run an AMS HT, its built-in heated drying keeps a TPU spool usable between jobs instead of needing a separate dryer.
Step 3: Choose the feeding path for your hardness
This is the step most guides skip, and it is where most TPU failures start. Match the path to the grade:
- Shore 68D — standard AMS path. TPU for AMS is the only TPU engineered to run through a standard AMS, AMS Lite or AMS 2 Pro, including multi-colour jobs. It is firm enough not to buckle in the long PTFE path. No other TPU should go through these units. (New to the AMS ecosystem? See our AMS setup guide.)
- Shore 95A — AMS HT. The AMS HT has a dedicated TPU outlet that gives 95A-grade flexibles a short, direct path with drying on board. If you are weighing it against the AMS 2 Pro, our AMS 2 Pro vs AMS HT comparison breaks down which suits flexible-heavy workflows.
- Shore 85A–95A HF — TPU Feed Assist Module. The Bambu Lab TPU Feed Assist Module (compatible with the P1, X1, H2 and P2S/X2D series) actively helps soft filament into the toolhead, which noticeably lifts success rates and surface quality on the softer grades.
- External spool holder — always works. On the A1 and A1 Mini, or any machine without the accessories above, feed soft TPU from the external spool holder for the shortest, straightest path, and print from a dry box if you can.
Step 4: Bambu Studio settings that actually matter
Bambu Studio ships sound TPU profiles, so start from the preset for your exact grade and adjust from there:
- Nozzle temperature: 220–240°C. Run the lower end for soft grades to reduce stringing, the upper end if layers are not bonding.
- Bed: around 30–45°C on the textured PEI plate. TPU bonds aggressively — a thin layer of liquid glue acts as a release agent so you do not damage the part (or the plate) getting it off. The fundamentals in our first layer guide apply here too, just in reverse: with TPU the challenge is letting go.
- Speed: slow and steady. Soft grades like to run at a fraction of PLA speeds; consistent slow extrusion beats bursts of fast movement every time.
- Retraction: 0.8–1.2 mm. More retraction than this on a flexible filament compresses the strand instead of pulling it back, which causes jams rather than curing strings.
- Flow and pressure: if you see gaps or blobs after drying and slowing down, run Bambu Studio's flow calibration on the actual spool.
Troubleshooting quick reference
| Symptom | Most likely cause | Fix |
|---|---|---|
| Hissing, popping, rough surface | Wet filament | Dry 8+ hours at ~70°C; store sealed |
| Heavy stringing | Moisture first, then temperature | Dry the spool, drop nozzle temp toward 220°C — then see our stringing guide |
| Clicking, filament wrapped in extruder | Buckling — wrong feed path or too fast | Shorten the path (external spool / feed assist), slow down |
| Jams only on soft grades | Retraction too long | Reduce to 0.8–1.2 mm |
| Part fused to plate | TPU over-adhesion | Liquid glue as release layer, cool plate fully before removal |
Two more things people get wrong about flexible printing
FDM TPU is not the same as resin "flexible". Flexible resins exist for SLA printers, but FDM TPU is in a different class for tear strength and fatigue life — a TPU hinge or strap survives flexing cycles that would split a flexible resin part. For functional flexible parts, FDM TPU is the default choice, not the compromise.
Foamed TPU is a different product category. The ultra-light cushioned TPU in commercial shoe midsoles and insoles is foamed during manufacture. Printed TPU can approximate cushioning through infill tricks, but it is not the same material behaviour — worth knowing before you promise someone printed orthotics.
Ready to print flexible?
Every TPU grade above — from 68D down to 85A — ships from our Sydney warehouse in Regents Park with fast Australia-wide delivery, alongside the full filament range and Bambu Lab printers and accessories. As an authorised Bambu Lab reseller and Australia's authorised Bambu Lab service centre, we print with these materials every day — if you are unsure which grade or feeding setup fits your job, talk to us. For current pricing on any printer or accessory mentioned here, see the Bambu Lab Australia price list.
FAQ
Can I print TPU through the AMS on a Bambu Lab printer?
Only Bambu Lab TPU for AMS (Shore 68D) is designed for the standard AMS, AMS Lite and AMS 2 Pro. Softer grades need the AMS HT's TPU outlet, the TPU Feed Assist Module, or an external spool — running them through a standard AMS is the fastest way to a tangle inside the unit.
Which TPU is easiest for a first-time flexible print?
TPU for AMS (68D) if you want zero workflow changes, or TPU 95A HF if you want a genuinely rubbery part — the HF (high flow) formulation tolerates higher speeds than classic 95A, so it is the most forgiving of the soft grades.
Do I need an enclosure to print TPU?
No. TPU has very low warping tendency and prints happily on open-frame machines like the A1 and A1 Mini. Enclosure requirements are an ABS/ASA concern, not a TPU one.
Why does my TPU print fine for an hour and then fail?
Usually moisture regain mid-print: in coastal Australian humidity a spool sitting in open air absorbs water while the job runs. Print long TPU jobs from a dry box or an AMS HT with drying active.
Can I print TPU and PLA in the same model?
They can be printed in one multi-material job but they barely bond to each other — which is occasionally useful (print-in-place without fusing) but means a TPU-over-PLA grip can peel off. Mechanical interlocks beat relying on layer adhesion between the two.